JIS | AISI | WNr | DIN |
SKS3 | O1 | 1.2510 | 1.2510 |
CHEMICAL COMPOSITION(Typical Analysis %)
C | Si | Mn | Cr | V | W |
0.95 | 0.25 | 1.10 | 0.60 | 0.10 | 0.60 |
STEEL PROPERTIES
Cold work tool steel. Very high resistance to cracking. High machinability, medium toughness and resistance to wear. Dimensional stability at heat treatment
PHYSICAL PROPERTIES
Thermal coductivity W/(m.K) 20°C/30
Density g/cm3 20°C/7.85
Coefficient of linear thermal expansion
10-6 °C-1 | 20-100°C | 20-200°C | 20-300°C | 20-400°C | 20-500°C | 0-600°C | 20-700°C |
---|---|---|---|---|---|---|---|
12.1 | 12.9 | 13.3 | 14.0 | 14.4 | 14.8 | 14.9 |
APPLICATIONS
Working tools, cutting blades, sizing and stamping tools
HEAT TREATMENT
SOFT ANNEALING(°C) | COOLING | HARDNESS (HB) |
740-770 | FURNACE | MAX. 230 |
HARDENING FROM(°C) | IN | HARDNESS AFTER QUENCHING (HRC) |
780-820 | OIL, AIR, THERMAL BATH 180-220°C | 64 |
TEMPERING (°C) | 200 | 300 | 400 | 500 | 600 |
HARDNESS (HRC) | 61 | 56 | 51 | 44 | 37 |
ADDRESS
PHH METAL 1 SDN. BHD.
Wisma PHH, Jalan PPU 3,
Taman Perindustrian Puchong Utama,
47100 Selangor,
Malaysia..
CONTACTS
Email: info@phh.com.my
: sales@phh.com.my
Telephone: +60 3 8068 7000
Fax: +60 3 8068 2020
LINKS